Calculators
What an electrode designation means: AWS A5.1 and EN ISO 2560-A
Type the class printed on the box — E7018-1 H4R or E 42 4 B 42 H5 — and we explain every part: strength, impact energy, covering, current, positions and hydrogen. For carbon-steel covered electrodes.
AWS A5.1 — carbon steel covered electrodes
| Symbol | Part | What it means |
|---|---|---|
| E | Product | Covered electrode for manual metal arc welding. |
| 70 | Tensile strength | At least 70 ksi; in AWS A5.1M, 490 MPa (class E49…). |
| 1 | Positions | All: flat, horizontal, vertical and overhead. |
| 18 | Covering and current | Basic, low hydrogen, potassium, with iron powder. Current: AC or DC+. |
| -1 | Improved toughness | Meets stricter impact-energy requirements than the class without «-1». E7016-1 and E7018-1: 27 J at −46 °C. |
| H4 | Diffusible hydrogen | At most 4 ml per 100 g of deposited weld metal. |
| R | Low moisture absorption | The covering has passed the AWS A5.1 moisture-absorption test. |
AC: alternating current. DC+: direct current, electrode positive. DC−: electrode negative.
In our catalogue, class E7018: 9 electrodes
Each electrode with its full designation, as the maker prints it.
- LASER B 47 · GedikOpen the page →E 7018 H4
- LASER B 50 · GedikOpen the page →E 7018 - 1 H4
- LASER B 55 · GedikOpen the page →E 7018 - 1 H4
- LASER B 55-S · GedikOpen the page →E 7018 - 1 H4
- LASER B 60 · GedikOpen the page →E 7018 - H4
- GARANT · KjellbergOpen the page →E 7018
- GARANT K · KjellbergOpen the page →E 7018-1
- GARANT S · KjellbergOpen the page →E 7018-1
- GARANT X · KjellbergOpen the page →E 7018-1
How to read an AWS A5.1 designation
| Symbol | Part | What it means |
|---|---|---|
| E | Product | Covered electrode for manual metal arc welding. |
| 60 | Tensile strength | At least 60 ksi; in AWS A5.1M, 430 MPa (class E43…). |
| 70 | Tensile strength | At least 70 ksi; in AWS A5.1M, 490 MPa (class E49…). |
| 1 | Positions | All: flat, horizontal, vertical and overhead. |
| 2 | Positions | Flat and horizontal fillet. |
| 4 | Positions | Flat, horizontal, overhead and vertical-down. |
| 10 | Covering and current | Cellulosic, sodium |
| 20, 22 | Covering and current | Iron oxide |
| 11 | Covering and current | Cellulosic, potassium |
| 12 | Covering and current | Rutile (titania), sodium |
| 13 | Covering and current | Rutile (titania), potassium |
| 14, 24 | Covering and current | Rutile (titania) with iron powder |
| 15 | Covering and current | Basic, low hydrogen, sodium |
| 16 | Covering and current | Basic, low hydrogen, potassium |
| 27 | Covering and current | Iron oxide with iron powder |
| 18, 28, 48 | Covering and current | Basic, low hydrogen, potassium, with iron powder |
| 19 | Covering and current | Iron oxide and rutile (titania), potassium |
| -1 | Improved toughness | Meets stricter impact-energy requirements than the class without «-1». E7016-1 and E7018-1: 27 J at −46 °C. |
| H4 | Diffusible hydrogen | At most 4 ml per 100 g of deposited weld metal. |
| H8 | Diffusible hydrogen | At most 8 ml per 100 g of deposited weld metal. |
| H16 | Diffusible hydrogen | At most 16 ml per 100 g of deposited weld metal. |
| R | Low moisture absorption | The covering has passed the AWS A5.1 moisture-absorption test. |
| M | Military requirements | Class with additional US military requirements; it carries no H4 or R mark. |
Covering, current and positions of the common classes
| Class | Covering and current | Positions |
|---|---|---|
| E6010 | Cellulosic, sodium. Current: DC+. | All: flat, horizontal, vertical and overhead. |
| E6011 | Cellulosic, potassium. Current: AC or DC+. | All: flat, horizontal, vertical and overhead. |
| E6012 | Rutile (titania), sodium. Current: AC or DC−. | All: flat, horizontal, vertical and overhead. |
| E6013 | Rutile (titania), potassium. Current: AC, DC+ or DC−. | All: flat, horizontal, vertical and overhead. |
| E6027 | Iron oxide with iron powder. Current: see the electrode's data sheet; for this class the sources disagree. | Flat and horizontal fillet. |
| E7014 | Rutile (titania) with iron powder. Current: AC, DC+ or DC−. | All: flat, horizontal, vertical and overhead. |
| E7016 | Basic, low hydrogen, potassium. Current: AC or DC+. | All: flat, horizontal, vertical and overhead. |
| E7018 | Basic, low hydrogen, potassium, with iron powder. Current: AC or DC+. | All: flat, horizontal, vertical and overhead. |
| E7024 | Rutile (titania) with iron powder. Current: AC, DC+ or DC−. | Flat and horizontal fillet. |
AC: alternating current. DC+: direct current, electrode positive. DC−: electrode negative.
How to read an EN ISO 2560-A designation
Yield, tensile strength and elongation
| Symbol | What it means |
|---|---|
| 35 | Yield strength ≥ 355 MPa; tensile strength 440–570 MPa; elongation ≥ 22 %. |
| 38 | Yield strength ≥ 380 MPa; tensile strength 470–600 MPa; elongation ≥ 20 %. |
| 42 | Yield strength ≥ 420 MPa; tensile strength 500–640 MPa; elongation ≥ 20 %. |
| 46 | Yield strength ≥ 460 MPa; tensile strength 530–680 MPa; elongation ≥ 20 %. |
| 50 | Yield strength ≥ 500 MPa; tensile strength 560–720 MPa; elongation ≥ 18 %. |
Impact energy
| Symbol | What it means |
|---|---|
| Z | No impact-energy requirement. |
| A | At least 47 J average at +20 °C. |
| 0 | At least 47 J average at 0 °C. |
| 2 | At least 47 J average at −20 °C. |
| 3 | At least 47 J average at −30 °C. |
| 4 | At least 47 J average at −40 °C. |
| 5 | At least 47 J average at −50 °C. |
| 6 | At least 47 J average at −60 °C. |
Chemical composition of the weld metal
| Symbol | What it means |
|---|---|
| — | No symbol: carbon-manganese steel, Mn ≤ 2.0 %. |
| Mo | Mn ≤ 1.4 %; Mo 0.3–0.6 % |
| MnMo | Mn 1.4–2.0 %; Mo 0.3–0.6 % |
| 1Ni | Mn ≤ 1.4 %; Ni 0.6–1.2 % |
| Mn1Ni | Mn 1.4–2.0 %; Ni 0.6–1.2 % |
| 2Ni | Mn ≤ 1.4 %; Ni 1.8–2.6 % |
| Mn2Ni | Mn 1.4–2.0 %; Ni 1.2–2.6 % |
| 3Ni | Mn ≤ 1.4 %; Ni 2.6–3.8 % |
| 1NiMo | Mn ≤ 1.4 %; Mo 0.3–0.6 %; Ni 0.6–1.2 % |
| Z | Any other agreed composition. «Z» electrodes may not be interchangeable. |
Covering
| Symbol | What it means |
|---|---|
| A | Acid |
| C | Cellulosic |
| R | Rutile |
| RR | Rutile, thick |
| RC | Rutile-cellulosic |
| RA | Rutile-acid |
| RB | Rutile-basic |
| B | Basic |
Efficiency and current
| Symbol | What it means |
|---|---|
| 1 | Electrode efficiency up to 105 %; alternating and direct current (AC and DC). |
| 2 | Electrode efficiency up to 105 %; direct current only (DC). |
| 3 | Electrode efficiency over 105 % up to 125 %; alternating and direct current (AC and DC). |
| 4 | Electrode efficiency over 105 % up to 125 %; direct current only (DC). |
| 5 | Electrode efficiency over 125 % up to 160 %; alternating and direct current (AC and DC). |
| 6 | Electrode efficiency over 125 % up to 160 %; direct current only (DC). |
| 7 | Electrode efficiency over 160 %; alternating and direct current (AC and DC). |
| 8 | Electrode efficiency over 160 %; direct current only (DC). |
Positions
| Symbol | What it means |
|---|---|
| 1 | All positions (PA, PB, PC, PD, PE, PF, PG). |
| 2 | All except vertical-down (PA, PB, PC, PD, PE, PF). |
| 3 | Flat and horizontal fillet (PA, PB). |
| 4 | Flat (PA). |
| 5 | Flat, horizontal fillet and vertical-down (PA, PB, PG). |
Diffusible hydrogen
| Symbol | What it means |
|---|---|
| H5 | At most 5 ml per 100 g of deposited weld metal. |
| H10 | At most 10 ml per 100 g of deposited weld metal. |
| H15 | At most 15 ml per 100 g of deposited weld metal. |
In EN ISO 2560-A the first five parts are compulsory; efficiency and current, positions and hydrogen are optional.
Basis: EN ISO 2560:2020 (system A) and AWS A5.1/A5.1M. The designation is the maker's declaration; this page explains the symbols and does not replace the standard or the electrode's data sheet.
← All calculators