Gedik · Creep-resisting Cr-Mo steels
OPUS MOB — E 7018-A1 H4
covered electrode · stick electrodebasic coating
Choose the size
- Ø 2.5 × 350 mm≈ 5 kg
- Ø 3.2 × 350 mm≈ 5 kg
- Ø 4 × 450 mm≈ 5 kg
- Ø 5 × 450 mm≈ 5 kg
To order · price and lead time in the quote
We reply within 1 working day.
How much filler metal do I need?With this product's data: 111 · η 0.55–0.65
Thickness of the plates to be joinedref. 1.3: 3 < t ≤ 10
Sum of all identical welds
6.97–11.14 kg
of OPUS MOB for 10 m of weld
3 packs of ≈ 5 kg
Calculated with: η 0.55–0.65: typical value for process 111 · preparation per EN ISO 9692-1 · EN ISO 5817 level C
See the full calculation →Do I need to preheat?With this product's data: H5
Thickness of the thickest part in the jointmethod B: d from 10 to 90 mm
100 °C
Minimum preheat and minimum interpass temperature
EN 1011-2, annex C, method B · rounded up to 5 °C
✓ Within the range of method B.
Calculated with: HD 5 ml/100 g from this product's class H5 · 111 — basic electrode: 24 V, 160 A, 15 cm/min
See the full calculation →Field of application
- Basic-coated stick electrode
- Welding of heat-resisting, Mo-alloyed, thin-walled and unalloyed steels used for construction of boilers and pipes
- Weld metal is resistant to working temperatures from -50°C to +550°C Re-drying: 300-350°C min. 2h
Base metals
S355J2G3E295E335P255G1TH16Mo3L320-L415NBL290MB-L415MBS255N-S460NP295GHP355GH15NiCuMoNb5S20MnMoNi4-517MnMoV6-4S255NH-S460NHS255NL-S460NLGE240-GE300GS22Mo4
| Positions | PA flat PB horizontal-vertical PC horizontal PD horizontal-overhead PE overhead PF vertical-up |
|---|---|
| Polarity | DC+ |
Classification and approvals
Classification
| AWS class | E 7018-A1 H4 |
|---|---|
| EN ISO class | E Mo B 42 H5 |
Approvals
- TÜV, DB, CE, SEPRO
According to the Gedik 2023 catalogue; validity is confirmed with the order
Composition and properties
Chemical composition of the weld metal
| C | 0.07 |
|---|---|
| Mn | 0.90 |
| Mo | 0.50 |
| Si | 0.40 |
Values in mass %.
Mechanical properties
| Service temperature | max. 550 °C |
|---|
after heat treatment: 620 °C / 1 h / 300 °C (air)
| Yield strength (Rp0.2) | min. 460 MPa |
|---|---|
| Tensile strength (Rm) | 530–670 MPa |
| Elongation (A5) | min. 22 % |
| Impact energy (KV) | min. 47 J (−50 °C) |
How to weld
Treatment and preparation
| Re-drying | 300–350 °C / min. 2 h |
|---|
Welding parameters by diameter
| Ø | Length | Current |
|---|---|---|
| 2.5 mm | 350 mm | 80–110 A |
| 3.2 mm | 350 mm | 100–140 A |
| 4 mm | 450 mm | 140–190 A |
| 5 mm | 450 mm | 190–240 A |
FERVEO guidance
By problem
Structural steels
Alternatives in the catalogue
Same class
same AWS designation · same EN ISO designation