Nickel-base electrode for joining and cladding on matching nickel-chromium-molybdenum steels and similar nickel-chromium steels, (heat-resisting) Cr and CrNi (Mo, N) steels and nickel-alloyed pressure vessel steels tough at low temperatures. Use at service temperatures from -196 °C up to 1,000 °C (in sulphur-containing atmospheres only up to 500 °C). The fully austenitic weld metal is corrosion-resisting, tough at low temperatures, with high-temperature strength, resistant to scaling up to 1,000 °C and not susceptible to embrittlement. High resistance to corrosive media.
Classification
AWS class
ENiCrMo-3
EN ISO class
E Ni 6625 (NiCr22Mo9Nb)
Materialno.(W.-Nr.)
2.4621
Chemical composition of the weld metal
C
Cr
Mn
Mo
Nb
Ni
Si
0.04
22.0
0.20
9.00
3.50
balance
0.25
Values in mass %.
Base metals
1.4529X1NiCrMoCuN25-20-7 · 1.4876X10NiCrAlTi32-21 · 2.4816 NiCr 15 Fe · 2.4856 NiCr 22 Mo 9 Nb · 2.4858 NiCr 21 Mo · Alloy 600 · Alloy 625 · Alloy 800 · Alloy 825
Mechanical properties
Yield strength (Rp0.2)
> 420 MPa
Tensile strength (Rm)
> 760 MPa
Elongation (A5)
> 30 %
Impact energy (KV)
> 90 J (room temperature) · > 40 J (−196 °C)
FERVEO IBERICA, S.L.U. · NIF B05613559 · Avda. del Tomillar, 70, 29631 Benalmádena (Málaga) · Registered in the Registro Mercantil de Málaga, sheet MA-201214 · info@ferveo.eu · www.ferveo.eu · FT-FINOX-625-EN · rev. 2 · page 1 / 2
Typical values, not guaranteed: this document is not a declaration of performance and does not replace the manufacturer's official documentation or the applicable WPS.
Prepared by FERVEO from the Kjellberg 2019 catalogue
FERVEO IBERICA, S.L.U. · NIF B05613559 · Avda. del Tomillar, 70, 29631 Benalmádena (Málaga) · Registered in the Registro Mercantil de Málaga, sheet MA-201214 · info@ferveo.eu · www.ferveo.eu · FT-FINOX-625-EN · rev. 2 · page 2 / 2
Typical values, not guaranteed: this document is not a declaration of performance and does not replace the manufacturer's official documentation or the applicable WPS.
Prepared by FERVEO from the Kjellberg 2019 catalogue