We open on 1 January 2027. Until then we are not accepting registrations or requests.
Datasheetas published in the maker's catalogueCross-referencesacross makers and AWS / EN ISO classesDeliverySpain and PortugalESPTEN
FERVEO
Basket
Kjellberg · Stainless steels

FINOX 4829 AC — E 309-17

covered electrode · stick electroderutile coating

Choose the size

  • Ø 2.5 × 300 mm · 4 kg
    ≈ 4 kg
  • Ø 3.25 × 350 mm · 5 kg
    ≈ 5 kg
  • Ø 4 × 350 mm · 5 kg
    ≈ 5 kg
To order · price and lead time in the quote

We reply within 1 working day.

How much filler metal do I need?With this product's data: 111 · η 0.55–0.65
Thickness of the plates to be joinedref. 1.3: 3 < t ≤ 10
Sum of all identical welds

7.02–11.21 kg

of FINOX 4829 AC for 10 m of weld

3 packs of 4 kg

Calculated with: η 0.55–0.65: typical value for process 111 · preparation per EN ISO 9692-1 · EN ISO 5817 level C

See the full calculation →

Field of application

Electrode for joining and surfacing on matching or similar heat-resisting steels and cast steels up to 950 °C. Particularly suitable for the steel X 15 CrNiSi 20 12 (1.4828).

Base metals

1.4710 GX 30 CrSi71.4713 X 10 CrAlSi71.4724 X 10 CrAlSi131.4740 GX 40 CrSi171.4742 X 10 CrAlSi181.4826 GX 40 CrNiSi 22-101.4828 X 15 CrNiSi 20-121.4833 X 12 CrNi 23-131.4878 X 8 CrNiTi 18-10AISI 309
PositionsPA flat PB horizontal-vertical PC horizontal PE overhead PF vertical-up
PolarityDC+/AC

Classification and approvals

Classification

AWS classE 309-17
EN ISO classE 22 12 R 32
Material no. (W.-Nr.)1.4829

Composition and properties

Chemical composition of the weld metal

C0.10
Cr22.5
Mn0.70
Ni12.5
Si0.80
Values in mass %.

Mechanical properties

Yield strength (Rp0.2)> 350 MPa
Tensile strength (Rm)> 550 MPa
Elongation (A5)> 30 %
Impact energy (KV)> 55 J (room temperature)

How to weld

Treatment and preparation

Re-drying300–350 °C / 2 h

Storage

In the original packaging, in dry, ventilated rooms: 5–30 °C, relative humidity < 60 %, up to 2 years.

Moisture in the coveringMore spatter and porosity: redry, above all when low hydrogen content is required.
According to the Kjellberg 2019 catalogue

Welding parameters by diameter

ØLengthCurrent
2.5 mm300 mm70–100 A
3.25 mm350 mm100–140 A
4 mm350 mm130–170 A
FERVEO guidance
By problem
Dissimilar metalsStainless steel and dissimilar metalsCorrosion-resistant alloys