Choose the size
- Ø 0.8 mm · K300 15–20 kg≈ 15 kg
- Ø 1 mm · K300 15–20 kg≈ 15 kg
- Ø 1.2 mm · K300 15–20 kg≈ 15 kg
- Ø 1.6 mm · K300 15–20 kg≈ 15 kg
Indicative diameters; confirmed with the order
Supply programme: spools on request D100 (0.5–1 kg), D200 (2–5 kg)
To order · price and lead time in the quote
We reply within 1 working day.
How much filler metal do I need?With this product's data: 135 · η 0.92–0.98
Thickness of the plates to be joinedref. 1.3: 3 < t ≤ 10
Sum of all identical welds
4.62–6.66 kg
of DT-SG Mo MIG for 10 m of weld
1 pack of ≈ 15 kg
Calculated with: η 0.92–0.98: typical value for process 135 · preparation per EN ISO 9692-1 · EN ISO 5817 level C
See the full calculation →Field of application
Joint welding in apparatus, vessel, boiler and pipeline construction. Service temperature up to +550 °C.
Base metals
St 35.8St 45.8HIHII17Mn1419Mn615Mo316Mo3GS-C25GS-22Mo4WStE 255-WStE 460
| Polarity | DC+ |
|---|---|
| Shielding gas | M1, M2, M3, C1 |
Classification and approvals
Classification
| AWS class | ER70S-A1 |
|---|---|
| EN ISO class | G MoSi |
| Material no. (W.-Nr.) | 1.5424 |
Approvals
- TÜV, DB, CE
According to the Dratec 2025 catalogue; validity is confirmed with the order
Composition and properties
Chemical composition of the wire
| C | 0.10 |
|---|---|
| Mn | 1.10 |
| Mo | 0.50 |
| Si | 0.60 |
Values in mass %.
Mechanical properties
guide values
| Yield strength (Rp0.2) | 490–520 MPa |
|---|---|
| Tensile strength (Rm) | 560–650 MPa |
| Elongation (A5) | > 22 % |
| Impact energy (KV) | > 80 J |
| Service temperature | −40–550 °C |
FERVEO guidance
By problem
Structural steels
Alternatives in the catalogue
Same class
same EN ISO designation
| Product | Class | Rm | KV | Availability |
|---|---|---|---|---|
| SG Mo MIGGedik | G MoSi | 550–670 MPa | min. 47 J (−20 °C) | To order · price and lead time in the quote |