FINOX 29/9 GOLD — ≈ E 312-16
Choose the size
- Ø 2.5 × 300 mm · 4 kg≈ 4 kg
- Ø 3.25 × 350 mm · 5 kg≈ 5 kg
- Ø 4 × 350 mm · 5 kg≈ 5 kg
We reply within 1 working day.
Field of application
FINOX 29/9 Gold is a special electrode for extremely crack-resistant joining and surfacing on difficult-to-weld steels, e.g. austenitic manganese steel, tool steel and spring steel, and for dissimilar joints, e.g. between ferritic and austenitic steels. Owing to its good mechanical properties and corrosion resistance, the electrode has a wide range of applications in the repair and maintenance of machine and plant components, e.g. shafts and gears, and for tools. The electrode is equally suitable for buffer layers under hard alloys. Thanks to its stable arc, the electrode has excellent welding characteristics and forms a finely rippled, easily controlled bead, with very good slag detachability. The all-weld metal is stainless and work-hardenable when cold and hot.
| Positions | PA flat PB horizontal-vertical PC horizontal PE overhead PF vertical-up |
|---|---|
| Polarity | DC+/AC |
Classification and approvals
Classification
| AWS class | ≈ E 312-16 |
|---|---|
| EN ISO class | E Z 29 9 R 12 |
| EN 14700 class | E Fe 11 |
| Material no. (W.-Nr.) | ≈ 1.4337 |
Approvals
- CE
Composition and properties
Chemical composition of the weld metal
| C | 0.10 |
|---|---|
| Cr | 30.0 |
| Mn | 1.00 |
| Ni | 9.50 |
| Si | 0.70 |
Mechanical properties
| Yield strength (Rp0.2) | > 640 MPa |
|---|---|
| Tensile strength (Rm) | > 800 MPa |
| Elongation (A5) | > 20 % |
How to weld
Treatment and preparation
| Re-drying | 300–350 °C / 2 h |
|---|
Storage
In the original packaging, in dry, ventilated rooms: 5–30 °C, relative humidity < 60 %, up to 2 years.
| Moisture in the covering | More spatter and porosity: redry, above all when low hydrogen content is required. |
|---|
Welding parameters by diameter
| Ø | Length | Current |
|---|---|---|
| 2.5 mm | 300 mm | 80–110 A |
| 3.25 mm | 350 mm | 100–140 A |
| 4 mm | 350 mm | 130–170 A |