Carbon equivalent in welding: formula and calculation of CE (IIW), CET and Pcm

Enter the composition from your 3.1 certificate and get the three carbon equivalents used by the welding standards. The higher the value, the more prone the steel is to cold cracking and the more preheat it needs. For carbon and low-alloy steels.

Steel
Composition, % by mass
Used by Pcm only. 20 ppm = 0.0020 %.
The steel standard's values: the middle of the range where the standard gives a minimum and a maximum; the maximum of C, Si and Mn where it gives only a maximum; the other elements at 0. Replace them with your certificate's.

CE (IIW)

0.403 %

CE (IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15 = 0.17 + 1.4/6 + (0 + 0 + 0)/5 + (0 + 0)/15 = 0.403 %

The IIW formula. Used by EN 1011-2 (method A) and by product standards: it is the CEV of EN 10025-2.

Range of EN 1011-2 method A: C 0.05–0.25 %; Si ≤ 0.8 %; Mn ≤ 1.7 %; Cr ≤ 0.9 %; Ni ≤ 2.5 %; Mo ≤ 0.75 %; Cu ≤ 1.0 %; V ≤ 0.20 %

✓ Within the range of method A.

CET

0.310 %

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40 = 0.17 + (1.4 + 0)/10 + (0 + 0)/20 + 0/40 = 0.310 %

EN 1011-2, method B: with the thickness, the diffusible hydrogen and the heat input it gives the preheat temperature.

Range of EN 1011-2 method B: C 0.05–0.32 %; Si ≤ 0.80 %; Mn 0.50–1.90 %; Cr ≤ 1.50 %; Ni ≤ 2.50 %; Mo ≤ 0.75 %; Cu ≤ 0.70 %; V ≤ 0.18 %; CET 0.20–0.50 %

✓ Within the range of method B.

Pcm

0.240 %

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5·B = 0.17 + 0/30 + (1.4 + 0 + 0)/20 + 0/60 + 0/15 + 0/10 + 5·0 = 0.240 %

Ito and Bessyo's parameter for low-carbon steels. Used by AWS D1.1 (hydrogen control method) and ISO 3183 (line pipe).

For Pcm we give no range per element: see the carbon rule.

Maximum CEV of S235JR to EN 10025-2 (thickness up to 30 mm): 0.35 %. The values above come from the standard's maximums, not from your steel's actual composition.

Which value to use

C = 0.17 %, over 0.12 %: use CE (IIW). ISO 3183 uses CE (IIW) above 0.12 % C.

For the preheat temperature to EN 1011-2, the input is CET.

Calculate preheat with this composition →

Three formulas, three uses

Formula, % by massWhere it is used
CE (IIW)CE (IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15The IIW formula. Used by EN 1011-2 (method A) and by product standards: it is the CEV of EN 10025-2.
CETCET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40EN 1011-2, method B: with the thickness, the diffusible hydrogen and the heat input it gives the preheat temperature.
PcmPcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5·BIto and Bessyo's parameter for low-carbon steels. Used by AWS D1.1 (hydrogen control method) and ISO 3183 (line pipe).

AWS D1.1 uses another CE variant with silicon: C + (Mn + Si)/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15. Here, the IIW one, as in EN 1011-2 and EN 10025.

We give no «good or poor weldability» scale: the sources disagree on the limits, and the risk also depends on the thickness, the consumable's hydrogen and the heat input. The preheat calculation takes those into account.

Basis: EN 1011-2:2001 + A1:2003, annex C (methods A and B); Ito and Bessyo, IIW Doc. IX-576-68; AWS D1.1:2025, annex B; ISO 3183. Indicative result: it does not replace the standard or the welding procedure (WPS).